7. Example: Thermocuring of Epoxy Resin - a Comparison of Different Reaction Types
For a homogeneous system, we’ve already discussed in detail the characteristic reaction progress for different Reaction typesReaction type is the elementary mechanism of one individual reaction step in multi-step chemical reaction. Reaction type f(Cr, Cp) describes dependence of the reaction rate for individual reaction step on the concentrations of reactant Cr and product Cp for this step.reaction types (n-th order, auto-catalysis, and combined auto-catalysis). Here we will use a DSC example of the curing of epoxy resin. By comparing the kinetics model-fit results, we are trying to help our customers understand the difference between these reaction types visually and intuitively.
Here we carried out DSC tests on curing process of epoxy resin at different heating rates (5, 10, 20 K/min), and obtained the following exothermal curing peaks. The experimental curves are present in the Figure 6:

There are some articles which prove that the curing of epoxy resin (EP) is some kind of auto-catalysis reaction [3]. However, here we will put all of these existing conclusions aside and suppose we don’t know what’s going on chemically inside of the material at all. We will therefore try to apply different reaction types to carry out curve-fitting, and decide what the possible reaction type is from the fit quality alone.

In the Fig.7, the points are measured data points, and the lines are calculated fit-optimized curves using n-th order reacton type (Fn). We already know that the DSC signal is directly proportional to the reaction rate.
If we compare the fit curve with the measured curve and focus on the early stage, we find that the n-th order reaction has no obvious induction period and the increase in the reaction rate is relatively smooth. While for the measured signal, the starting part is more horizontal and the later acceleration is more strong (the left side of the peak is sharper than for the fit curve). This indicates that the reaction can involve an auto-catalysis mechanism.

In Fig.8 we will attempt to use the pure auto-catalysis Prout-Tompkins reaction type, namely Bna, to carry out a curve fit. The overall fit quality is greatly improved, but the early stage of reaction is still not so properly fitted. If we focus on the solid line (fit curve), we’ll find that the pure auto-catalysis function has a longer induction period during which the reaction rate is close to zero (nearly a horizontal line); after that, the reaction rate accelerates faster than it does in reality.

Finally, we will use the combined auto-catalysis reaction Cn to carry out a curve fit. In Fig.9, the calculated curve fits almost perfectly with the measured curve. This indicates that the reaction mechanism might possibly be a combination of n-th order and auto-catalysis paths:

with weighting factor Kcat=1.34. Other parameters listed here:
Ea = 46.2 kJ/mol
lgA = 2.5 lg(1/s)
n = 1.7
All these values are in a chemically sensible range, which proves this reaction type is reasonable.